Butyl Tape Data Sheet: Peel Adhesion, Shear & Temperature Test Data

图片1butyl_tape_peel_adhesion_test_setup
图片3butyl_tape_membrane_joint_pressure_roller
图片1butyl_tape_peel_adhesion_test_setup
图片3butyl_tape_membrane_joint_pressure_roller

This butyl tape data sheet compares peel, shear, creep and temperature data for unsupported, reinforced and foil-faced butyl seals. Force readings depend on specimen geometry, substrate, conditioning and failure mode. The published figures represent independent grades, not this site’s verified specifications. Confirm the actual joint with representative specimens. Report the substrate finish, preparation, load and environmental exposure, because nominal readings alone cannot determine suitability.

The Specimen Must Be Defined Before the Force

Unsupported butyl can stretch or split; reinforcement redistributes force. Record thickness, backing, liner removal and clamping.

Match the specimen structure against the butyl sealant tape range before comparing figures.

Record failure locus.

Peel Strip, Loaded Lap or Compressed Seal?

Test Item

What It Checks

Suggested Method or Reference

Why It Matters

When To Request It

Peel adhesion

Interface separation

ASTM D3330 if applicable; H41 internal

Geometry sensitivity

New substrate

Dynamic shear

Rapid shear

H15 internal

Not creep

Grade changes

Static holding

Slow slip

ASTM D3654 if applicable

Load duration

Loaded joints

Sealant tensile

Bond/cohesive failure

ASTM C907 if applicable

Failure locus

Compressed joints

Membrane T-peel

Film separation

H45; 250 um membrane

Steel differs

Membrane changes

For peel, record substrate, width, speed, dwell and failure locus; internal H-methods are not ASTM equivalents.

Published Numbers Kept With Their Original Grades

Item

Typical Value / Reference Range

Test Method or Condition

Notes

Total thickness

1.0 mm [E, F]

Published grades

Grade-specific

180-degree peel

8 [A], 11 [B], 14 [C] N/cm

Internal H41

Match dwell

180-degree peel to stainless steel

60 [E1], 50 [E2] N/25mm

JIS Z 0237:2000, as cited

Different structures

90-degree peel

7 [A], 11 [B], 7 [C] N/cm

Internal H48

Angle-dependent

Dynamic shear

12 [A-C], 13 [D] N/cm2

Internal H15

Not holding time

Membrane T-peel

12 N/cm [D]

H45; 250 um membrane

Film-dependent

Tensile elongation

200% [E1], 9% [E2]

JIS Z 0237:2000, as cited

Different structures

Service temperature

-20 to +60 C [B]; -40 to +90 C [A, D]; -40 to +110 C [C]

Published grade ratings

Not installation range

A Strong Peel Can Still Conceal Slow Joint Movement

Peel is not a seal test; rapid shear cannot predict creep. Service-temperature ratings exclude installation limits and outdoor life.

Steel-panel results may differ from membrane bonding. Test double-sided butyl vapor barrier tape on the actual film.

Record film treatment, pressure and dwell against a control.

A Membrane Coupon Needs Its Own Observation Record

At 24 h, 72 h and 7 days, inspect compression and spread as optional checkpoints.

Inspect edge lift, migration, squeeze-out, bubbles, shadows and tears; record fracture location.

For alternate joint geometries, see industrial uses for butyl tape; verify the assembly separately.

Specify leak-test criteria.

Where a Number Can Mislead the Joint Decision

Data Point

If Too Low

If Too High

Risk in Application

Check Before Full Use

Thickness (E/F: 1.0 mm)

Gap underfill

Extrusion

Voids

Joint compression

Peel (A-C: 8/11/14 N/cm)

Edge release

Coating disturbance

Interface mismatch

Matched peel test

Dynamic shear (A-D: 12/13 N/cm2)

Weak rapid-load resistance

Creep unproven

Creep risk

Static-load trial

Elongation (E1/E2: 200%/9%)

Limited movement

Construction-dependent

Backing damage

Confirm construction

Service limit (B/C: +60/+110 C)

Poor heat margin

Life unproven

Flow

Aging test

Preserve Exposure History Alongside the Result

Record grade, lot, liner, storage and compression history.

Compare exposed rolls with controls; record fixture and operator.

FAQ

How should I compare peel figures in a butyl tape data sheet?

Match angle, surface, speed and dwell; units alone are insufficient.

Will a high peel force confirm a watertight compressed joint?

No. Test the compressed joint for leakage and movement.

What should a creep record capture that dynamic shear misses?

Log load, area, temperature, duration, slip and censored results.

When should a stored or transported roll be retested?

Compare suspect rolls with retained controls.

Scroll to Top

Get A Free Quote Now !

Contact Form Demo (#3)